The influence of Aluminum on the iron-carbon system with Si-S-Mg presence.
Thermocalc, TCFE6.1, Fe-C (0-5% Al)
An interesting case was studied a complex alloy, its composition is shown in the table.
Composition Alloy
Content wt%
|
Si |
S |
Mg |
C |
Al |
3.4 |
0.008 |
0.045 |
3.1 |
0-4 |
Legend (Phases):
- Liquid
- Liquid-Graphite
- Liquid-FCC_A1
- Graphite-FCC_A1
- FCC_A1
- BCC_A2-FCC_A1
- FCC_A1-BCC_A2-Graphite
- BCC_A2-Graphite
- Liquid-BCC_A2
- Liquid-BCC_A2-FCC_A1
- Liquid-FCC_A1-Graphite
- FCC_A1-Graphite-Kappa
- BCC_A2-FCC_A1-Kappa
- FCC_A1-Kappa
- BCC_A2-Kappa
- Liquid-Graphite-Kappa
- Liquid-FCC_A1-Kappa
- Liquid-Kappa
Ideas
- Austenitic region is small.
- This region grows up with the Aluminum content.
- There is not carbides precipitation.
- The aluminum content change the eutectic point.
Profile critical points
The next table and graphic show the temperature and composition variation with Aluminum content in the system.
Critical Points
Al(%wt) |
Peritectic |
Eutectic |
C (%wt) |
T (°C) |
C (%wt) |
T (°C) |
0.5 |
0.3146 |
1397 |
3.302 |
1185 |
1 |
0.331 |
1398 |
3.282 |
1203 |
2 |
0.359 |
1398 |
3.217 |
1229 |
2.5 |
0.373 |
1397 |
3.177 |
1238 |
3 |
0.386 |
1395 |
3.135 |
1246 |
3.5 |
0.398 |
1393 |
3.09 |
1252 |
4 |
0.411 |
1390 |
3.044 |
1257 |
T (°C)
%wt.C
Changed: 22.09.2009